Having smashed my fairings into eight pieces, it was time for repair. I like the OEM "road-worn" look. So, instead of buying a whole new set of fairings, I decided to just clean mine up. After some research, the results were quite good. Total cost was ~$90 and it took one day:

MATERIAL CONSIDERATIONS
The fairings are made of BASF Terblend N. It's a mix of fibrelgass, ABS and PA, styrenic polymers, and nylon. For paints/gloss to bond properly, they need to be in the same chemical family as the substrate. This is why paint from a enamel rattle spray won't dry properly on fairings. The workaround is to use an intermediate layer that connects the different materials, ie an adhesion promoter, more on that down below.

JOINING BROKEN PIECES AND FILLING CRACKS
Sand all edges, wipe down with denatured alcohol, use Loctite Plastic Epoxy to fill cracks. Then use the epoxy and fiberglass cloth to join the pieces from behind. Easiest way is to re-cut the cloth to the shape you need, mix and wipe the epoxy on the cloth like knife on bread, and put into place. Dries to a very strong yet flexible bond. I tried many different epoxy systems over the past couple years and this one has performed the best. Be sure to wipe any epoxy drips that managed to leak into front of fairing. If there's any left after it dries, and you plan to paint, scrape with a razor blade at 90 degree angle. Sanding will only make it worse because the fairing material is softer than the epoxy.

COLOR MATCHING
Do this first because it can make a big difference in the end. You have to decide whether you want a very close match or note. I plan to sell my bike soon, so I wanted it as close as possible. I contacted a local auto paint shop who also has a store front. They guys were life savers. Before I drove over, I held some paint swatches near my fairings to find a good match. I happen to have a Pantone swatchbook, but if you don't, just go down to Home Depot and take a bunch of their glossy paint swatches. For my job, my front fairings needed a blue match, so I brought the swatch that matches that to these guys. He looked at it and said he could match it but if its a bike, it probably has some pearlescence. So he went back into his back room and mixed up a match with that and 20 minutes later handed me a spray can he put it into, $25. I love service like that, and the colormatch was very very close.

SANDING
Dry sand throws the material everywhere, so sand all surfaces down with 400 grit wet/dry. I had tons of scratches on my main white fairing, some very deep. I was able to remove most of them by going down to 120 grit and then back up. I did not go the bondo route, but you can if you want super smooth contours. Beneath the color is black material and this is important for the white fairings. For deep scratches, go slow and light. The scratch will clear up, but if you go too hard the black will be exposed beneath. And careful around the edges where sanding angles pull off paint faster, its easy to go overboard there.

PAINT AND CLEAR COAT
For BASF Terblend N is special, the shop advised the following:
- Tape angles with blue 3m tape and to prevent overspray
- Wipe with denatured alcohol. Careful on the decals because they will bleed.
- Spray light coat with Bulldog Adhesion Promotor, let dry to tack 5 mins, hit it again a bit heavier. Dry 20 mins.
- Color coat: spray one light coat, let dry to tack 5 min. Repeat until you have good coverage. Don't go to heavy as it will orange peel. Let this dry for 30 minutes, assuming 70F with 50RF. Your tack/dry times will vary if the temp/humidity is different.
- USC Spray Max 2k  (two component) High Gloss Clearcoat Aerosol. This is this schizmit. It's a fast drying, two-component acrylic resin/isocyanate hardener. "Very high chemical, gasoline, and weather resistance for high-quality and long-term sealing of repair paint jobs and new paint jobs on cars and motorcycles."  It's actually two spray cans connected on the inside. You place a red disc on one side and smack it down, and it combines the two, good for 24 hours. Again, start with a light coat, dry to tack in 5 minutes, repeat until it builds up. I did 4 coats. It will look slightly dimpled, but lays down over 12 hours.

BUFF/WAX
They said the this coating will expand and shrink as it dries and off-gasses, so wait a month to do this. Some areas look showroom glossy while others have a bit orange peel, but only from certain angles. I will wet/dry with 1500/2000 grit to bring this down, then buff wax.

SAFETY NOTES
The adhesive and the 2k are quite nasty, so be sure to wear a good respirator. I was horrified at how much is caked on the filter after I take it off. A tyvek suit, booties, and head wrap prevents you from tracking the stickiness and fumes everywhere, only ~$10.

Rashed, the "before" pic------->https://imgur.com/a/ZiQgE
Pic of cowling during reconstruction------->https://imgur.com/a/n2CdN
Pic of cowling , the "after" pic, Area above finger is factory, are below finger is DIY. -------> https://imgur.com/a/b0pEn
"Spray booth"------>https://imgur.com/a/65rRp
Finished, still need to mount the blinkers---->https://imgur.com/a/eaA7Y



2007F with 22k NY/NJ miles. Stock exhaust/airbox. Rejet to 20/60/132/one o-ring/1.25 turns out, +2 mojo

Endopotential

That's a great writeup which will help a lot of people out there.   Mods, can we sticky this?  :cheers:
http://gstwins.com/gsboard/index.php?topic=70953.0

2007 GS500F Cafe Fighter - cut off the tail, K&N lunchbox, short exhaust, 20/60/140 jets, R6 shock, all sorts of other random bits...

gregjet

Shoo Goo will bond it pretty well permanantly and is petrol resistant.  8 pieces sounds like there would have been some deformation. It may self bend over time.
Don't know why they have such a complex mix when it obviously doesn't stay in one piece. Almost every faiting I have seen on Japanese bikes has a crack or break somewhere. If they made it out of proper Fibreglass at least it would be completely repairable.
Give us a progress report in 6 months and see if your method lasts. It would be nice to know something works on the stuff.

The Buddha

Fiberglass is brittle as duck.
But ABS, when you breal it, you have to buy new sheite from them ...
Remember there are 2 phases of jap crap in the 90's. 80 through the early 90's they wanted to make stuff that will last forever and they were in the "take over the world mode"
Then sometime in the early 90's as the economy began to collapse, they got into the "why aren't you buying new parts" mode.

The GS benefitted from the "we'll get to you later mode" till maybe 2000. Then in 01-02 they were confused. Then 04 onwards they truly went to the "why aren't you buying cheap plastic crap from us that we can charge 100X as uch" mode.
Cool.
Buddha.
-----------------------------------------------------------------
I run a business based on other people's junk.
-----------------------------------------------------------------

gregjet

The new material is glass/ innegra or carbon/innegra. The innegra increases the flexibility hugely ( don't put innegra on the outside though, as it doesn't finish well).
Yes glass , especailly a bit aged, is brittle, but even ridiculous damage can be repaired like nothng happened. Epoxy instead of polyester makes a huge difference is brittleness.